Test Data - Coating
| Property | Test Description | Results |
| Adhesion | Elcometer | <3000 psi 210 kg/cm2 |
| Adhesion to steel (Shear) | ASTM D 1002 10 mil (254 micron) glue line |
4300 psi 302kg/cm2 |
| Impact | Gardner 5/8 in (1,6 cm) diameter tup 1/8 in x 3 in x 3 in (0,32 cm x 7,6 cm) steel plate |
160 in-lbs 1,8 kg |
| Hardness | Barcol ASTM D 2583 | 23 |
| Abrasion Resistance |
ASTM D 1044 CS-17 1000 g weight 5000 cycles |
0,07 g loss |
| Thermal Shock |
310° to - 100°F (154° to -73°C) 4 in x 4 in (10,2cm x 10,2 cm) coated panel |
10 cycles no effect |
| Penetration | ASTM G 17 -40° to 240°F (-40°-116°C) |
0 |
| Tensile Strength |
ASTM D 2370 | 7300 psi 512kg/cm2 |
| Elongation Compressive Strength |
ASTM D 2370 ASTM D 695 |
4.2% 12800 psi 900 kg/cm2 |
| Coefficient of Friction | API RP5L2-1968, App8 | 23° |
| Electric Strength | ASTM D 149 | 1000 volts/mil 39,4 kv/mm |
| Hot Water Resistance |
160°F (71°C) immersion 120 days |
Good Adhesion. No blistering |
| Electrical Resistivity | ASTM D 257 | 1.2 x 1015 ohm |
| Thermal Conductivity | MIL-I-16923E | 7 x 10-4cal/sec/cm2/C°/cm |
| Water Absorption | 3M 10 mil (254 micron) free film 30 days | 6,5 g/m2 |
| Fungus Resistance | MIL-STD 810-B Method 508 | Funginert |
| Salt Fog | MIL-E-5272C | No Effect |
| Weatherometer | ASTM G 23 5000 hours | Surface chalk |
| Soil Stress - Burial | Bureau of Reclamation 25 cycles | No effect |
| Salt Crock | 30 day, 5 volt, 5% NaCl sand crock 23° F (110° C) |
Distbondment diameter 24 mm average |
| Bendability | 3/8 in (9,5 mm) coupon mandrel bend at 73° F (23° C) |
30 pipe diameters 1.9° /diameter length |